Tool Steels H26 is stocked by 1 North American distributors and produced by 1 large mills. Distributors will offer small quantity buys while mills will generally only sell large quantities, with delivery times anywhere from 10 to 50 weeks depending on size and form required
This material is stocked primarily in Bar Products by 1 distributors.
For distributor (small quantity) availability click here
For mill (large volume) production click here
To view all click here
Specifications
The following specifications cover Tool Steels H26
- ASTM A681 (H-28)
- UNS T20824
Property Results
Related Metals:
Chemistry Data : [top]
Carbon
|
|
0.45 - 0.55 |
Chromium
|
|
3.75 - 4.5 |
Manganese
|
|
0.15 - 0.4 |
Phosphorus
|
|
0.03 max |
Silicon
|
|
0.15 - 0.4 |
Sulphur
|
|
0.03 max |
Tungsten
|
|
17.25 - 19 |
Vanadium
|
|
0.75 - 1.25 |
Principal Design Features
|
|
This alloy is one of the Hot Work, higher tungsten content with chromium and vanadium tool steels. It has good resistance to softening when used in hot applications.
|
|
Applications
|
|
Applications are those that involve hot forming temperatures such as hot extrusion or forming dies.
|
|
Machinability
|
|
Machinability of H26 is medium. It rates at 60% that of the W group (rated 100%) water hardening low alloy tool steels.
|
|
Forming
|
|
The alloy may be formed by conventional methods.
|
|
Welding
|
|
This alloy is weldable. Consult the supplier for details.
|
|
Heat Treatment
|
|
Preheat to 1600 F and then raise temperature rapidly to 2225 F. Hold for 2 to 5 minutes at temperature and then air cool, oil, or salt bath quench.
|
|
Forging
|
|
Forge at 2100 F down to 1775 F. Do not forge below 1750 F.
|
|
Hot Working
|
|
See "Forging".
|
|
Cold Working
|
|
H26 may be cold formed by conventional methods.
|
|
Annealing
|
|
Anneal at 1625 F and slow cool at 40 F maximum per hour.
|
|
Aging
|
|
Not applicable to this alloy.
|
|
Tempering
|
|
Temper at 1050 F to 1250 F for Rockwell C of 58 to 43. A double (repeat) temper is advised for best results.
|
|
Hardening
|
|
See "Heat Treatment" and "Tempering".
|
|
Physical Data : [top]
|
|
Density (lb / cu. in.)
|
0.318
|
Specific Gravity
|
8.8
|
Melting Point (Deg F)
|
2610
|
Modulus of Elasticity Tension
|
30
|
Mechanical Data : [top]
MSO currently has no data available for this grade.
|
Videos :
MSO currently has no videos available for this grade.
|
Disclaimer
This information is provided "as is" and Metal Suppliers Online, Inc. makes no warranty of any kind with respect to the subject matter or accuracy of the information contained herein. Metal Suppliers Online, Inc. specifically disclaims all warranties, expressed, implied or otherwise, including without limitation, all warranties of merchantability and fitness for a particular purpose.
In no event shall Metal Suppliers Online, Inc. be liable for any special, incidental, indirect or consequential damages of any kind or any damages whatsoever resulting from loss of use, data, profits, whether or not advised of the possibility of damage, and on any theory of liability, arising out of or in connection with the use of the information contained herein.
This publication may include technical inaccuracies or typographical errors. Changes may be periodically made to the information herein.